MPIF STANDARD 35
2016 Edition
Materials Standards for
MetalInjectionMolded Parts2016
MPIF Standard 35
Standards Materials Injection Metal for Molded Parts*
*See MPIF Standard 35, Materials Standards for PM Structural Parts for structural parts made by the powder metallurgy (PM) process.
*See MPIF Standard 35, Materials Standards for PM Self-Lubricating Bearings for bearings and bushings made by the PM process.
*See MPIF Standard 35, Materials Standards for P/F Steel Parts for steel
components made by the powder forging (PF) process.
Table of Contents—2016 Edition
EXPLANATORY NOTES AND DEFINITIONS Minimum Value Concept .................................................................................. 3 Minimum Mechanical Property Values ............................................................ 3 Minimum Magnetic Property Values ............................................................. 3 Minimum Controlled-Expansion Property Values ........................................ 3 Practical Methods of Demonstrating Part Performance ................................................................................................. 3 Typical Values ......................................................................................................... 4 Chemical Composition...................................................................................... 4 Mechanical Properties ...................................................................................... 4 Heat Treatment ....................................................................................................... 4 Surface Finish ................................................................................................................ 4 Microstructure .......................................................................................................... 4 MIM Material Designation ................................................................................. 4 Material Selection .................................................................................................... 4 Grade Selection ...................................................................................................... 5 Density ........................................................................................................... 5 Ultimate Tensile Strength ................................................................................. 5 Yield Strength .......................................................................................................... 5 Elongation .......................................................................................................................... 5 Elastic Constants .................................................................................................... 5 Young’s Modulus (E) ........................................................................................ 5 Shear Modulus (G) ................................................................................................. 5 Poisson’s Ratio (?) ................................................................................... 5 Impact Energy ................................................................................................................ 5 Macroindentation Hardness (Apparent) ........................................................... 5 Microindentation Hardness ........................................................................... 6 Corrosion Resistance ....................................................................................... 6 Sulfuric Acid Testing ...................................................................................... 6 Copper Sulfate Testing .................................................................................. 6 Boiling Water Testing ..................................................................................... 6 Soft Magnetic Properties .................................................................................. 6 Magnetizing Field (H) ..................................................................................... 6 Induction (B) ......................................................................................................... 6 Maximum Induction (Bm) ............................................................................... 6
Maximum Permeability (μ max)
....................................................................... 6 Coercive Field (Hc) ......................................................................................... 6 Residual Induction (Br)................................................................................... 6 Thermal Properties ................................................................................... 7 Coefficient of Thermal Expansion (CTE) ........................................................ 7 Thermal Conductivity ................................................................................ 7 SI Units .......................................................................................................... 7 Referenced MPIF Standards .................................................................... 7 Comparable Standard ...................................................................................... 7 DATA TABLES – INCH-POUND UNITS Low-Alloy Steels .................................................................................................. 8-9 Stainless Steels ........................................................................................ 10-11 Soft-Magnetic Alloys ............................................................................... 12-13 Controlled-Expansion Alloys .................................................................. 14-15 Copper .............................................................................................. 16-17 DATA TABLES – SI UNITS Low-Alloy Steels ....................................................................................... 18-19 Stainless Steels ........................................................................................ 20-21 Soft-Magnetic Alloys ................................................................................. 22-23 Controlled-Expansion Alloys .................................................................. 24-25 Copper .............................................................................................. 26-27 1? i
INDEX Alphabetical Listing & Guide to Material Systems &
Designation Codes Used in MPIF Standard 35 ......................................... 28
SI UNITS CONVERSION TABLE Quantities/Terms Used in MPIF Standards ................................................ 33
2?ii
MPIF Standard 35 Materials Standards for
Metal Injection Molded Parts
Issued 1993 Revised 2000, 2007 and 2016 Scope MPIF Standard 35 is issued to provide the design and materials engineer with the information necessary for specifying powder metal (PM) materials that have been developed by the PM parts manufacturing industry. This section of Standard 35 deals with products manufactured by Metal Injection Molding (MIM). It does not apply to conventional PM structural materials, PM self-lubricating bearings or powder forged (PF) materials which are covered in separate editions of MPIF Standard 35. Each section of this standard is divided into subsections based on the various types of MIM materials in common commercial use within that section. Notes at the beginning of each subsection discuss the characteristics of that material. The same materials may appear in more than one section of the standard depending upon their common use, e.g., some low-alloy or stainless steel materials may also be used in soft-magnetic applications. The use of any MPIF Standard is entirely voluntary. MPIF Standards are issued and adopted in the public interest. They are designed to eliminate misunderstandings between the manufacturer and the purchaser and to assist the purchaser in selecting and obtaining the proper material for a particular product. Existence of MPIF Standards does not in any respect preclude any member or non-member of MPIF from manufacturing or selling products that use materials or testing procedures not included in MPIF Standards. Other such materials may be commercially available. By publication of these Standards, no position is taken with respect to the validity of any patent rights nor does the MPIF undertake to ensure anyone utilizing the Standards against liability for infringement of any Letters Patent or accept any such liability. Neither MPIF nor any of its members assumes or accepts any liability resulting from use or non-use of any MPIF Standard. In addition, MPIF does not accept any liability or responsibility for the compliance of any product with any standard, the achievement of any minimum or typical values by any supplier, or for the results of any testing or other procedure undertaken in accordance with any Standard. MPIF Standards are subject to periodic review and may be revised. Users are cautioned to refer to the latest edition. New, approved materials and property data may be posted periodically on the MPIF website. Between published editions, go to mpif.org to access data that will appear in the next printed edition of this standard. Both the purchaser and manufacturer should, in order to avoid possible misconceptions or misunderstandings, agree on the following conditions prior to the manufacture of a MIM component: material selection, chemical composition, minimum property values and any other processes, that may affect the part application. No part of this publication may be reproduced, stored in a retrieval system, or transmitted, in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior permission of the publisher. ? Copyright 2016 ISBN No. 978-1-943694-05-1 Published by
Metal Powder Industries Federation
105 College Road East
Princeton, New Jersey 08540-6692 U.S.A.
Tel: (609) 452-7700Fax: (609) 987-8523E-mail: info@mpif.org
Website: mpif.org
1?
No part of this publication may be reproduced, stored in a retrieval system, or transmitted, in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior written permission of the publisher ISBN No. 978-1-943694-05-1 ? 2016 Metal Powder Industries Federation 105 College Road East Princeton, New Jersey 08540-6692 USA All rights reserved Produced in the U.S.A. 2?
MPIF Standard 35—2016 Materials Standards for Metal Injection Molded Parts Explanatory Notes and Definitions
Minimum Value Concept
The Metal Powder Industries Federation has adopted the concept of minimum property values for metal injection molded (MIM) materials. These values may be used to determine the material best suited to the particular application as it is manufactured by the metal injection molding (MIM) process.
As an aid to the user in selecting materials, in addition to minimum property values, typical values for other properties are listed. This makes it possible for the user to select and specify the exact MIM material and properties most suitable for a specific application. The data provided define minimum values for listed materials and display typical properties achieved under commercial manufacturing procedures. Enhanced mechanical properties and other improvements in performance characteristics may be attained through more complex processing. To select a material optimum in both properties and cost effectiveness, it is essential that the part application be discussed with the MIM parts manufacturer.
Minimum Mechanical Property Values
The minimum mechanical property values for MIM materials are expressed in terms of yield strength (0.2% offset method), ultimate tensile strength and percent elongation for all materials in the as-sintered and/or heat treated conditions. MIM materials exhibit properties similar to wrought materials because they are processed to near full density.
The tensile properties utilized for establishing this Stan-dard were obtained from tensile specimens prepared spe-cifically for evaluating MIM materials. Tensile properties of test specimens machined from commercial parts or from non-standard MIM test specimens, may vary from those obtained from specimens prepared according to MPIF Standard 50. (See MPIF Standard 50 for additional details)
Minimum Magnetic Property Values
The minimum magnetic property values for MIM materials are expressed in terms of part density, maximum permeability, maximum coercive force and magnetic saturation. The specified minimum magnetic saturation is measured with an applied field of 25 oersteds. All magnetic test data reported are for DC testing only.
The magnetic properties utilized for establishing this Standard were obtained from specimens prepared and tested in accordance with ASTM A773.
Minimum Controlled-Expansion Property Values A minimum density level is expressed for the MIM controlled-expansion alloys due to their use in electronics applications to provide hermetic seals with materials such as glasses and ceramics.
Practical Methods of Demonstrating Part Performance
For structural parts, the practical method of demonstrating minimum values is through the use of a static or dynamic proof test by the manufacturer and the purchaser using the first production lot of parts and a mutually agreed upon method of stressing the part. For example, from the design of a given part, it is agreed that the breaking load should be greater than a given force. If that force is exceeded in proof tests, the minimum strength is demonstrated. The first lot of parts can also be tested in service and demonstrated to be acceptable. The static or dynamic load to fracture is determined separately and these data are statistically analyzed to determine a minimum breaking force for future production lots. Exceeding that minimum force on future lots is proof that the specified strength has been met.
For parts that require minimum magnetic characteristics, the practical method of demonstrating acceptable mag-netic properties is through the use of a magnetic proof test. For example, from the design of a given part, it is agreed that the magnetic force generated by the part when a specified magnetic field is applied should be greater than a mutually agreed upon value between the parties concerned. If that force is exceeded in proof tests, the minimum magnetic performance is demonstrated. Exceeding this minimum value on future lots is proof that the specific magnetic properties have been met.
Utilization of MPIF Standard 35 to specify a MIM material means that unless the purchaser and manufacturer have agreed otherwise, the material will have the minimum value specified in the Standard. (See Material Properties section.)
3?
MPIF Standard 35, Metal Injection Molded Parts—2016 Edition Typical Values Most MIM materials respond well to normal wrought For each MIM material listed, a set of typical values is heat treating practices and procedures. It is recommended shown for properties, e.g., density, hardness, elongation, that the heat-treatment procedures for any MIM etc., some or all of which may be important for a specific material be established in cooperation with the MIM application. Typical values are shown for properties, part manufacturer to achieve the desired balance of e.g., elongation, hardness, coercive field, etc., some or final properties in the finished part. all of which may be important for a specific application. The property data were compiled from test specimens Surface Finish processed by individual MIM producers. The overall finish and surface reflectivity of MIM materi-The typical values are listed for general guidance als depends on density, tool condition, particle size and only. They should not be considered minimum values. secondary operations. Effective surface smoothness of While achievable through normal manufacturing as-sintered MIM components is usually better than an processing, they may vary somewhat depending upon investment cast surface. Surface finish can be further the area of the component chosen for evaluation, or improved by secondary operations such as coining, the specific manufacturing process utilized. Those honing, burnishing or grinding. The surface finish properties listed under the “typical value section” for requirements and methods of determination must be each material which are required by the purchaser established by mutual agreement between purchaser should be thoroughly discussed with the MIM parts and producer. (See MPIF Standard 58 for additional manufacturer before establishing the specification. details.) Required property values, other than those expressed as minimum should be separately specified for each Microstructure MIM part, based on its intended use. MIM materials generally contain less than 5% porosity, approaching the density of wrought materials. Chemical Composition The examination of the microstructure of a MIM part The chemical composition of each material lists its can serve as a diagnostic tool and reveal the degree of principal elements and allowable ranges. sintering and other metallurgical information critical to the metal injection molding process. There are several Mechanical Properties observations common to most sintered MIM materials, Mechanical property data indicate the minimum and as briefly described below. Comments on specific typical properties that may be expected from test materials will be found in the subsections devoted to specimens conforming to the density and chemical those particular materials. composition criteria listed. It should be understood that Sintered parts are normally examined first in the mechanical properties used in this standard were unetched condition. With a proper sinter, there will be derived from individual test specimens prepared no original particle boundaries seen at 200X. Small, specifically for material evaluation and sintered under uniformly distributed, well rounded discrete pores lead commercial production conditions. to higher strength, ductility and impact resistance. Hardness values of heat treated specimens are given first as apparent hardness and second, when available, MIM Material Designation as equivalent particle or matrix hardness values. The Metal Injection Molding Association has chosen Residual porosity found in MIM components will slightly to use the designation system similar to AISI-SAE affect the apparent hardness readings. Microin-where applicable. These designations were chosen
dentation hardness values shown as Rockwell C were because MIM parts are likely to be used as converted from 100 g load (0.981 N) Knoop microin-replacements for wrought products already in service.
dentation hardness measurements. When specifying a material made by the MIM process, it should be so designated with a “MIM” prefix to the Heat Treatment material grade. For example, a part fabricated from MIM materials may be heat treated to increase strength, Type 316L stainless steel by MIM would be designated hardness and wear resistance. The percentages of car-as \
bon, alloying elements and residual porosity determine the degree of hardening possible. Tempering or stress Material Selection relief is required after quenching for optimum strength Before a particular material can be selected, a careful and durability. Ferrous MIM parts processed with little analysis is required of the design of the part and its or no final carbon may be surface carburized for end use. In addition, the final property requirements of increased surface hardness while retaining core the finished part should be agreed upon by the toughness. Martensitic and precipitation hardening manufacturer and the purchaser of the MIM part.
Issues such as static and dynamic loading, wear stainless steels may also be heat treated for increased
resistance, machinability and corrosion resistance may hardness and strength.
also be specified.
4?
Grade Selection
For certain magnetic materials, the material designation will specify the material as either “Grade 1” or “Grade 2”. The Grade 1 material, as compared with Grade 2, will exhibit improved magnetic characteristics. The difference between a Grade 1 and Grade 2 material can usually be found in the material’s microstructure, with a high density, large grain size and low amounts of interstitials (carbon, oxygen, nitrogen, etc.) all contributing to improved magnetic properties. A careful analysis of the design and function of the part should determine what grade material is required for a given application. It is recommended that a discussion of the required magnetic performance take place between the manufacturer and the purchaser before the final grade selection.
Density
Density is expressed in grams per cubic centimeter
3
(g/cm) and may be determined by various standardized methods. Some common methods of MIM density deter-mination include:
MPIF Standard 54: This method is generally used for products that contain less than 2% porosity (impermeable PM). It is based on the principle of water displacement.
MPIF Standard 63: This method comprises use of a gas pycnometer. Any open porosity will not be included as part of measured volume. The density obtained by the gas pycnometer method will typically be higher than the density obtained by water displacement.
MPIF Standard 42: This method is generally used for PM products having surface-connected porosity and is based on the use of Archimedes’ principle. MIM materials generally contain less than 5% porosity, so impregnation is not applicable. Ultimate Tensile Strength Ultimate tensile strength, expressed in 103 psi (MPa) is the ability of a test specimen to resist fracture when a pulling force is applied in a direction parallel to its longitudinal axis. It is equal to the maximum load divided by the original cross-sectional area. (See MPIF Standard 50 for additional details.) Yield Strength Yield Strength, expressed in 103 psi, is the load at which a material exhibits a 0.2% offset from proportionality on a stress-strain tension curve divided by the original cross-sectional area. (See MPIF Standard 50 for additional details.)
MPIF Standard 35, Metal Injection Molded Parts—2016 Edition
Elongation Elongation (plastic), expressed as a percentage of the original gage length (typically 1.0 in. [25.4mm]), is based on measuring the increase in gage length after fracture, providing the fracture takes place within the gage length.
Elongation can also be measured with a break-away extensometer on the tensile specimen. The recorded stress strain-curve displays total elongation (elastic and plastic). The elastic strain at the 0.2% yield strength must be subtracted from the total elongation to give the plastic elongation. (See MPIF Standard 59 for additional details.)
Elastic Constants Data for the elastic constants in this standard were generated from resonant frequency testing. An equation relating the three elastic constants is:
Young’s Modulus (E)
Young’s modulus, expressed in 106 psi (GPa), is the ratio of normal stress to corresponding strain for tensile or compressive stresses below the proportional limit of the material. Shear Modulus (G) Shear modulus, expressed in 106 psi (GPa), is the ratio of shear stress to corresponding shear strain below the proportional limit of the material. Poisson’s Ratio (?) Poisson’s ratio is the absolute value of the ratio of transverse strain to the corresponding axial strain resulting from uniformly distributed axial stress below the proportional limit of the material. Impact Energy Impact energy, measured in foot-pounds-force (Joules), is a measure of the energy absorbed in fracturing a specimen in a single blow. An unnotched 5 mm X 10 mm cross- section Charpy specimen was used to establish the MIM impact energy values. (See MPIF Standard 59 for additional details.) Macroindentation Hardness (Apparent) The hardness value of a MIM part when using a conventional indentation hardness tester is referred to as \hardness\because it represents a combination of matrix hardness plus effect of residual porosity. The effect of residual porosity on hardness values is minor for MIM parts. Apparent hardness measures the resistance to indentation.
5?
MPIF Standard 35, Metal Injection Molded Parts—2016 Edition The manufacturer and the purchaser should agree on
the hardness, the measuring procedure, and the
hardness scale for each part tested. (See MPIF
Standard 43 for additional details.)
Microindentation Hardness Microindentation hardness is determined by utilizing Knoop (HK) or Vickers (HV) indentors with a microinden-tation hardness tester. It measures the true hardness of the structure by eliminating the effect of porosity, and thus is a measure of resistance to abrasive and adhesive
wear. Microindentation hardness measurements are
convertible to equivalent Rockwell hardness values
for comparison with other materials. A description of the microstructure must be reported.
The specimen shall be polished to reveal the porosity
and lightly etched to view the phases in the micro-structure and to determine where to place the hardness indentation. If the indentor strikes an undisclosed pore,
the diamond mark will exhibit curved edges and the
reading must be discarded. Since the data tend to be
scattered compared with pore-free material, it is recom-mended that a minimum of 5 indentations be made, anomalous readings discarded, and an average taken of
the remainder. (See MPIF Standard 51 for additional
details.) Corrosion Resistance Three media and test methods were used to rate the resistance of the MIM stainless steel alloys to corrosion. Sulfuric Acid Testing - Standard 5 mm X 10 mm X 55 mm test specimens were immersed in a 2% sulfuric acid solution at room temperature (72 °F ± 4 °F [22 °C ± 2 °C])
for 1,000 hours. Two replicates were tested. The loss
in mass for each was determined and then
converted into a mass loss per surface area (in dm2)
per day factor, in units of
g
(dm2) (day)
(See MPIF Standard 62 for additional details.)
Copper Sulfate Testing - The copper sulfate test consists of mixing 22.5 ml of distilled water with 1 g cupric sulfate crystals and 2.5 g sulfuric acid. Specimens are immersed in this solution for 6 minutes at a temperature between 63 Specimens that show no visual ° and 67 signs °F (17 of copper ° and 19 plating °C). are classified as passing this test. (See ASTM F1089 for additional details.)
6
Boiling Water Testing - The boiling water test consists of immersing the specimen in boiling, distilled water for 30 minutes. After 30 minutes, the heat source is shut off and the specimen remains in the water for 3 hours. The specimen is then removed and left to dry for 2 hours. Specimens that show no visual corrosion are classified as passing this test. (See ASTM F1089 for additional details.)
Soft-Magnetic Properties The magnetic data presented in this standard were developed in accordance with ASTM Standard A773. Magnetizing Field (H) The magnetic field applied to a test specimen, measured in oersteds (Oe) or amperes/metre (A/m). Induction (B) The measured magnetic field generated in a test specimen due to an applied magnetic field, measured in kilo- gauss (kG) or tesla (T). Maximum Induction (Bm) The maximum value of induction in a DC hysteresis loop. This value depends on the magnetizing field applied. Data are reported at magnetizing fields of 25 Oe
and 500 Oe, (1,990 A/m and 39,800 A/m), in units of kilogauss (kG) or tesla (T). Maximum Permeability (μmax) The slope of the line from the origin to the knee of the initial B-H magnetization curve. This parameter is dimensionless.
Coercive Field (Hc) The DC magnetizing field required to restore the magnetic induction to zero after the material has been symmetrically, cyclically magnetized, measured in Oe (A/m).
Residual Induction (Br) The retained magnetism in the specimen after
the applied field has been reduced to zero Oe (A/m).
This is reported in kG or T.
MPIF Standard 35, Metal Injection Molded Parts—2016 Edition
Referenced MPIF Standards
The test method standards referenced in this document are published by MPIF and are available in the latest edition of Standard Test Methods for Metal Powders and Powder Metallurgy Products.
Std. 42 Density of Compacted or Sintered
Powder Metallurgy (PM) Products
Std. 43
Apparent Hardness of Powder Metallurgy Products
Preparing and Evaluating Metal
Injection Molded (MIM) Sintered/Heat Treated Tension Test Specimens Microindentation Hardness of Powder Metallurgy Materials
Density of Impermeable Powder Metallurgy (PM) Materials
Surface Finish of Powder Metallurgy (PM) Products
Charpy Impact Energy of Unnotched Metal Injection Molded (MIM) Test Specimens
Corrosion Resistance of MIM Grades of Stainless Steel Immersed in 2% Sulfuric Acid Solution
Density Determination of Metal
Injection Molded (MIM) Components (Gas Pycnometer)
Std. 50
Std. 51
Idealized Magnetic Hysteresis Curve
Reference: Soft Magnetism, Fundamentals for Powder Metallurgy and Metal Injection Molding, Chaman Lall, Metal Powder Industries Federation, 1992, p.11.
Std. 54
Std. 58
Thermal Properties
Coefficient of Thermal Expansion (CTE)
The fractional increase in the length per unit rise in temperature at constant pressure.
Thermal Conductivity
The rate of heat flow, under steady state conditions, through a unit area, per unit temperature gradient in the direction perpendicular to the area. Thermal conductivity was determined in accordance with ASTM E1461, thermal flash method.
SI Units
Data were determined in inch-pound units and con-verted to SI units in accordance with IEEE/ASTM SI 10.
Std. 59
Std. 62
Std. 63
Comparable Standard
Standards for metal injection molded parts have been issued by ASTM. The ASTM standard was adapted from MPIF Standard 35 and uses the MPIF MIM nomenclature system.
ASTM B883 Standard Specification for Metal
Injection Molded (MIM) Materials
Additional MIM materials and property data are under development. When available, data will be published in subsequent editions of this Standard.
New, approved materials and property data may be posted periodically on the MPIF website. Between published editions, go to mpif.org to access data that will appear in the next printed edition of this standard.
7
MIM Material Section—2016 MPIF Standard 35
Low-Alloy Steels from both prealloys and admixtures of iron powder and This subsection covers MIM materials manufactured Application
other and carbon.
alloying elements such as nickel, molybdenum, Low-alloy steels are generally used for structural applications, especially when carburized. They are specified for applications where high strength and treat The proportions of each element used and heat hardness are necessary.
properties. conditions Microstructure
strength Alloys may may be varied be hardened to achieve for a very range high of Residual pores should be small, discrete, well may with moderate ductility. Lower carbon alloys distributed and rounded. The microstructure will vary achieving a tough core.
be case hardened for wear resistance while with composition and heat treatment.
Material Characteristics
takes Complete diffusion of alloying elements structure place high imparts during exceptional sintering. strength The normally properties. homogeneous The gives these materials good ductility.
density attained through MIM processing also
Material Chemical Composition, % — Low-Alloy Steels Designation Code Fe Ni Mo C Cr Si (max) Mn (max) MIM-2200(1) Bal. 1.5 – 2.5 0.5 max 0.1 max – 1.0 – MIM-2700 Bal. 6.5 – 8.5 0.5 max 0.1 max – 1.0 – MIM-4140 Bal. – 0.2 – 0.3 0.3 – 0.5 0.8 – 1.2 0.6 1.0 MIM-4605(2)
Bal. 1.5 – 2.5 0.2 – 0.5 0.4 – 0.6 – 1.0 – Other Elements: Total may not exceed 1.0% combined.
(1) Formerly designated as MIM-4600 (2) Formerly designated MIM-4650 with the addition of a minimum 0.2% Mo. To select a material optimum in both properties and cost effectiveness, it is essential that the part application be discussed with the MIM parts manufacturer. (See Explanatory Notes: Minimum Value Concept.) Both the purchaser and manufacturer should, in order to avoid possible misconceptions or misunderstandings, agree on the following conditions prior to the manufacture of a MIM component: material selection, chemical composition, minimum property values and any other processes, that may affect the part application
8
sitnU dnuoPh-cnI – seirtepor Plaireat MMIM n) d o-ieottr Cra cteDDDDR////inv sMenlNNNNH lsdoe5encni(w5dnk)rca-oto inHotRB C B rae ctrRBRRCanaHRMepHHR Hdpna59 Hi(46628464 de hytcpcy f trag r)00 oapeAbl03500nh11554nCmn(?tfIEU Ss’En U 888sooi8822222Lstt.....AnsaaioR00000tsP VLnAoC C css ’ IiPtguilsnup00505s.....Yaud 688999TlEoo022222YM1 n )ohitcan gi06 2n1B551 so lneEi(itreph o dt)ir%s lgPen2p 870 ieYe.30013805r1312ltisS(1neTeh ttiags mnp 20040i4644te3262lr0UtS1y t3 ism5 nc66555.....e/Dg77777n)ohitnc gai00 11 % 2231 noitces-ssorc mm 01 x mm 5 dehcto n.)-n9u5 ndraa mdnoartf Sd eFIviPreMd eseesu (lanve ymgicreenpes ty cpS:aarEphTmICO )NA( .dardnats siht fo sesoprup eht rof denimreted toN D/N 6102 ,7002 ,0002 :desiveR 2991 :devoprpA Low-Alloy Steels 2016 Edition MIM Material Section—2016 MPIF Standard 35 Stainless Steels This subsection covers MIM materials manufactured MIM-430L Ferritic Grade from prealloyed or elementally blended stainless steels. This ferritic stainless steel combines good magnetic Included are austenitic, ferritic and precipitation hardening response with corrosion resistance. It is suitable for grades. applications in a corrosive environment where protective coatings are impractical. (See Soft-Magnetic Alloys Material Characteristics section for additional information about this material.) High densities achieved by the MIM process enhance the strength, ductility and corrosion resistance of these MIM-17-4 PH Precipitation Hardening Grade materials. The precipitation hardening grade of stainless is used where a high level of strength and hardness is Application necessary. It generally has better corrosion resistance There are several grades of MIM stainless steels. than the 400 series stainless steels because of low Each has specific properties which cover a wide variety of carbon content. A range of properties and hardness applications: can be achieved through modifications of the aging temperature during heat treatment. MIM-316L Austenitic Grade This grade is used in applications which require extremly good corrosion resistance. Parts made from Microstructure All materials should exhibit wrought-like microstructures this material have a good combination of strength and except that MIM materials have evenly dispersed, well ductility. rounded pores. There should be no evidence of original particle boundaries. Internal oxides, nitrides and chromium MIM-420 and MIM-440 Martensitic Grades carbides are detrimental to properties. These martensitic stainless steels combine high strength, hardness and wear resistance with moderate corrosion resistance. A range of properties and hardness can be achieved though modifications of the carbon content and heat-treating conditions. Material Designation Chemical Composition, % — Stainless Steels Code Fe Ni Cr Mo C Cu Nb Nb + Ta Mn (max)Si (max) MIM-316L Bal. 10 – 14 16 – 18 2 – 3 0.03 (max)–– –– –– 2.0 1.0 MIM-420 Bal. –– 12 – 14 –– 0.15 – 0.4–– –– –– 1.0 1.0 MIM-430L Bal. –– 16 – 18 –– 0.05 (max)–– –– –– 1.0 1.0 MIM-440 Bal. 0.6 (max) 16 – 18 0.75 (max)0.9 – 1.25–– 3.5 (max)–– 1.0 1.0 MIM-17-4 PH Bal. 3 – 5 15.5 – 17.5 –– 0.07 (max)3 – 5–– 0.15 – 0.45 1.0 1.0 Other Elements: Total may not exceed 1.0% combined. To select a material optimum in both properties and cost effectiveness, it is essential that the part application be discussed with the MIM parts manufacturer. (See Explanatory Notes: Minimum Value Concept.) Both the purchaser and manufacturer should, in order to avoid possible misconceptions or misunderstandings, agree on the following conditions prior to the manufacture of a MIM component: material selection, chemical composition, minimum property values and any other processes, that may affect the part application 10 sitnU dnuoPh-cnI – seirtepor Plaireat MMIM e clt)isssssnosOssssssae2saaaaatBTHa(PPPPPPiss4e ROsDssDsss//s SsnuaNaoCPPNaaPPm imds e o4d5450sdrO/520 r oSm0D26501aet13000 2./....xba CHd/0N000 .teg< <0